Propertya
|
Testb Method
|
Typical Value, Unitsc
|
 |
|
Plasticizer
|
|
12%
|
 |
|
Specific Gravity
|
D 792
|
1.20
|
 |
 |
| Mechanical Properties
|
 |
|
Tensile Stress @ Yield
|
D 638
|
31.7 MPa (4600 psi)
|
 |
|
Tensile Stress @ Break
|
D 638
|
33.1 MPa (4800 psi)
|
 |
|
Elongation @ Break
|
D 638
|
45%
|
 |
|
Flexural Modulus
|
D 790
|
1448 MPa (2.10 x 105 psi)
|
 |
|
Flexural Yield Strength
|
D 790
|
41.4 MPa (6000 psi)
|
 |
|
Rockwell Hardness, R Scale
|
D 785
|
78
|
 |
|
Izod Impact Strength, Notched
|
|
@ 23°C (73°F)
|
D 256
|
416 J/m (7.8 ft·lbf/in.)
|
|
@ -40°C (-40°F)
|
D 256
|
107 J/m (2.0 ft·lbf/in.)
|
 |
 |
| Thermal Properties
|
 |
|
Deflection Temperatured
|
|
@ 1.82 MPa (264 psi)
|
D 648
|
75°C (167°F)
|
|
@ 0.455 MPa (66 psi)
|
D 648
|
83°C (181°F)
|
 |
|
Vicat Softening Temperatured
|
D 1525
|
96°C (205°F)
|
 |
 |
| Permanence Properties
|
 |
|
Water Absorption, 24 h immersion
|
D 570
|
1.5%
|
 |
|
Soluble Matter Loss
|
D 570
|
0.1%
|
 |
|
Weight Loss on Heating
[72 hours @ 80°C (176°F)]
|
D 1562
|
0.4%
|
 |
 |
| Miscellaneous Propionate Properties
|
 |
|
Refractive Index, nD
|
D 542
|
1.46-1.49
|
 |
|
Light Transmissione
|
E 308
|
>90%
|
 |
|
Hazee
|
D 1003
|
<8.5%
|
 |
|
Specific Heat
@ 23°C (73°F)
|
DSC
|
1.26-1.67 kJ/kg·K (0.301-0.399 Btu/lb·°F)
|
 |
|
Thermal Conductivity
|
C 177
|
0.17-0.33 W/m·K (1.2-2.3 Btu·in./h·ft2·°F)
|
 |
|
Coefficient of Linear Thermal Expansion
|
D 696
|
11 - 17 x 10-5 mm/mm·°C (6 - 9 x 10-5 in./in.·°F)
|
 |
|
Mold Shrinkage
|
D 955
|
0.2-0.6%
|
 |
|
Dielectric Strength
|
D 149
|
11.8-18.7 kV/mm (300-475 V/mil)
|
 |
|
Dielectric Constant
1 MHz
|
D 150
|
3.3-3.8
|
 |
|
Dissipation Factor
1 MHz
|
D 150
|
0.01-0.15
|
 |
|
Volume Resistivity
|
D 257
|
1013 - 1015 ohm·cm
|
 |
 |
a Unless noted otherwise, all tests are run at 23oC (73oF) and 50% relative humidity.
b Unless noted otherwise, the test method is ASTM.
c Units are in SI or US customary units.
d Conditioned 4 hours @ 70°C (158°F)
e 1.52-mm (0.06 in.) thickness
|